UNS N08904 AISI 904L Stainless steel
This data sheet applies to stainless steel 904L / 1.4539 hot and cold rolled sheet and strip, semi-finished products, bars, rolled wire and profiles as well as seamless and welded tubes for pressure purposes.
Chemical plant, oil refinery, petrochemical plants, bleaching tanks for the paper industry, combustion gas desulfurisation plants, application in sea water, sulphuric and phosphoric acid. Due to the low C-content, the resistance to intergranular corrosion is also guaranteed in the welded condition.
Element | % Present (in product form) |
---|---|
Carbon (C) | 0.02 |
Silicon (Si) | 0.70 |
Manganese (Mn) | 2.00 |
Phosphorous (P) | 0.03 |
Sulfur (S) | 0.01 |
Chromium (Cr) | 19.00 - 21.00 |
Nickel (Ni) | 24.00 - 26.00 |
Nitrogen (N) | 0.15 |
Molybdenum (Mo) | 4.00 - 5.00 |
Copper (Cu) | 1.20 - 2.00 |
Iron (Fe) | Balance |
Product Form | ||||||||
---|---|---|---|---|---|---|---|---|
C | H | P | L | L | TW/TS | |||
Thickness (mm) Max. | 8.0 | 13.5 | 75 | 160 | 2502) | 60 | ||
Yield Strength | Rp0.2 N/mm2 | 2403) | 2203) | 2203) | 2304) | 2305) | 2306) | |
Rp1.0 N/mm2 | 2703) | 2603) | 2603) | 2603) | 2603) | 2503) | ||
Tensile Strength | Rm N/mm2 | 530 - 7303) | 530 - 7303) | 520 - 7203) | 530 - 7304) | 530 - 7305) | 520 - 7206) | |
Elongation min. in % | Jmin (Longitudinal) | - | 100 | 100 | 100 | - | 120 | |
Jmin (Transverse) | - | 60 | 60 | - | 60 | 90 |
Density at 20°C kg/m3 | 8.0 | |
---|---|---|
Thermal Conductivity W/m K at | 20°C | 12 |
Modulus of Elasticity kN/mm2 at | 20°C | 195 |
200°C | 182 | |
400°C | 166 | |
500°C | 158 | |
Specific Thermal Capacity at 20°C J/kg K | 450 | |
Electrical Resistivity at 20°C Ω mm2/m | 1.0 |