Standard of 440C Stainless Steel and Equivalent Steel Grades

CountryUSABS & DINJapan
StandardASTM A276EN 10088JIS G4303
GradesS44004/440CX105CrMo17/1.4125SUS440C

ASTM A276 440C Steel Chemical Composition and Equivalent’s

StandardGradeCMnPSSiCrMo
ASTM A276S44004/440C0.95-1.20≦1.00≦0.04≦0.03≦1.0016.0-18.0≦0.75
EN10088X105CrMo17/1.41250.95-1.20≦1.00≦0.04≦0.03≦1.0016.0-18.00.40-0.80
JIS G4303SUS 440C0.95-1.20≦1.00≦0.04≦0.03≦1.0016.0-18.0≦0.75

ASTM 440C Stainless Steel Mechanical Properties

Tempering Temperature (°C)Tensile Strength (MPa)Yield Strength 0.2% Proof (MPa)Elongation (% in 50mm)Hardness Rockwell (HRC)Impact Charpy V (J)
Annealed*75844814269HB max#
204203019004599
260196018304579
316186017404569
371179016604569

Physical Properties

GradeDensity (kg/m3)Elastic Modulus (GPa)Mean Coefficient of Thermal Expansion (mm/m/°C)Thermal Conductivity(W/m.K)Specific HeatElectrical Resistivity (nW.m)
0-100°C0-200°C0-600°Cat 100°Cat 500°C0-100°C (J/kg.K)
440 C765020010.110.311.724.2460600

Forging of 440C Stainless Steel

Preheat to 760oC – 820oC, then heat slowly and uniformly to 1050oC – 1150oC, hold until temperature is uniform throughout the 440c steel section and commence forging immediately. Do not overheat 440c stainless steel as this can cause a loss of toughness and ductility. Do not forge below 900oC. Finished forgings of SS 440c should be cooled slowly in a furnace, warm dry lime or ashes to room temperature and annealed immediately. Air cooling after forging may cause cracking of steel 440c.

 