Chemical Composition Limits | ||||||||
Weight% | C | Mn | Si | P | S | Cr | Ni | Al |
17-7PH | 0.09 max | 1.00 max | 1.00 max | 0.040 max | 0.030 max | 16.00-18.00 | 6.50-7.75 | 0.75-1.50 |
Material | Condition | Ultimate Tensile Strength (ksi) | 0.2 % Yield Strength (ksi) | Elongation % in 2D | % Reduction of Area | Rockwell C Hardness |
17-7 Sheet / Strip AMS 5528 | Cond A | 105 max | 65 | 20 | - | 92 HRB max |
17-7 Sheet / Strip AMS 5528 | TH1050 | 180-120 | 150 | 4-6 | - | 38-46 |
17-7 Sheet / Strip | RH950 | 220 | 200 | 9 | - | 46 |
17-7 Sheet / Strip AMS 5529 | Cond C | 200 min | 175 min | 1 | - | 41 min |
17-7 Sheet / Strip AMS 5529 | CH 900 | 240 min | 230 min | 1 | - | 46 min |
17-7 Bar AMS 5644 | Cond A | 170 min | 140 min | 6 | 25 | 363 HB min |