Opening Hours: Mon - Sat 8:00 - 18:00

X8CrNiMoAl15-7-2 1.4532 Stainless steel

Prouduct name: X8CrNiMoAl15-7-2 1.4532 Stainless steel

abstract: X8CrNiMoAl15-7-2 1.4532 Stainless steel

Popular in these Categories: stainless steel

Contact: +86-0571-86628016

Technical Data Sheet

Chemical Composition Limits
Weight%CMnSiPSCrNiMoAl
15-7Mo0.09110.040.0314-166.50-7.752-30.75-1.5

PH 15-7 Mo is a precipitation hardenening stainless steel used for applications requiring high strength and moderate corrosion resistance. It is similar to 17-7 with the substitution of 2% Molybdenum for 2% Chromium resulting in higher room and elevated temperature strength for 15-7 Mo. PH 15-7 Mo stainless steel may be formed in a soft austenitic condition and then hardened to high strength levels by low temperature heat treatments. This allows miminum distortion compared to other quench and temper hardening processes. For maximum strength requirements, 15-7 Mo strip can be supplied in the hard-rolled Condition C for heat treatment to condition CH900.

The heat treatment processes for 15-7 Mo Stainless Steel (AMS 5520/ UNS S15700) are as follows:

Solution Treatment: heat to 1950°F and air cool
TH1050 (AMS 5520)
Solution Treatment: heat to 1950°F and air cool
Austenite Condition: Heat to 1400°F and hold for 90 minutes and cool to 55°F within 1 hr and hold for 30 minutes
Precitipation Harden: Heat to 1050°F and hold for 90 minutes then air cool

RH950 (AMS 5520)
Solution Treatment: heat to 1950°F and air cool
Austenite Condition: Heat to 1750°, hold for 10 minutes and cool to room temperature. Then within 1 hour cool to -100°F, hold for 8 hours then warm in air to room temperature
Precitipation Harden: Heat to 950°F and hold for 90 minutes then air cool

CH900
Condition C: Condition A is transformed to martensite at the mill by cold reduction to Condition C
Fabricate
Precipitation Harden: Heat to 900°F (+/-10) and hold for 60 minutes then air cool

Typical Mechanical Properties

 

MaterialCondition
Thickness (in)Tensile Strength (ksi)Yield Strength (ksi)Elongation %Hardness
Alloy 15-7 Mo
Solution Treated<0.005150 (max)65 (max)25100 HB (max)
Alloy 15-7MoTH1050 (AMS 5520)0.010-0.020190170440 HRC
Alloy 15-7 MoTH1050 (AMS 5520)0.020-0.1875190170540 HRC
Alloy 15-7 MoTH1050 (AMS 5520)0.1875-0.500190170640 HRC
Alloy 15-7 MoRH950 (AMS 5520)0.010-0.020225220345 HRC
Alloy 15-7 MoRH950 (AMS 5520)0.020-0.1875225220445 HRC
Alloy 15-7 MoRH950 (AMS 5520)0.1875-0.500225220545 HRC
Alloy 15-7 MoCondition C-200175141 HRC
Alloy 15-7 MoCondition CH900-240230146 HRC

 